JABET Explore more articles

Table 2. Percentage of delignification in MAA pre-treated biomass and reducing sugar yield from the liquid wash obtained after pre-treatment.

Power (W)

Lignin (%, W/W)

Delignification percentage

Reducing sugar in the wash liquid from MAA (mg/mL)

 

Untreated

AVLR biomass

Treated

AVLR biomass

   

160

13.95 ± 0.45

8.06 ± 0.28***

44.14 ± 5.08

0.22 ± 0.05

320

13.95 ± 0.45

4.68 ± 0.06****

66.38 ± 0.31

0.33 ± 0.02

480

13.95 ± 0.45

8.51 ± 0.03***

38.92 ± 1.32

0.98 ± 0.11

           

The values are average of triplicate experiments and the standard deviation is represented as (±) calculated from mean and three independent trials. ****p < 0.0001 and ***p < 0.001.